G-AlSi7Mg Sandguss härten nach T6
| Festigkeitsvergleich | ||||||
| EN AC Legierung |
42000 G-AlSi7Mg |
42100 G-AlSi7Mg0,3 |
42200 G-AlSi7Mg0,6 |
42300 G-AlSi7(Mg) | ||
| Zustand | F | T6 | T6 | T64 | T6 | T6 |
| Dehngrenze Rp0,2 in MPa | 80 | 180 | 190 | 120 | 210 | 140 |
| Zugfestigkeit Rm in MPa | 140 | 220 | 230 | 200 | 250 | 200 |
| Bruchdehnung A50 in % | 2 | 1 | 2 | 4 | 1 | 3 |
| Härte 5-250 in HBW | 50 | 75 | 75 | 60 | 85 | 60 |